Fixing PETG stringing, in order
PETG is the filament I reach for when a part has to survive being dropped, warmed up or squeezed. It is also the one that grows spiderwebs between every pair of features. After a lot of test towers, the fixes that matter come in a fairly fixed order, and skipping ahead usually wastes a day.
Step 1: moisture
If the filament crackles or leaves a rough, matte surface, nothing in the slicer will fully cure it. Dry the spool first (the oven method at 60 °C works) and repeat the test. Roughly half of the stringing complaints I see disappear at this step.
Step 2: temperature
PETG oozes more as it gets hotter. Print a temperature tower from 250 down to 220 °C in 5-degree steps and look at which section is cleanest while still sticking between layers. Most spools end up between 225 and 240 °C. Below that range, layers may separate when you flex the part; above it, strings return. Choose the lowest temperature whose layers you cannot peel apart with a fingernail.
Step 3: retraction
Start with a conservative profile and change one value at a time:
- Direct drive: 0.8 mm at 30 mm/s is a good starting point; try up to 2 mm.
- Bowden tube: 4 mm at 40 mm/s; go up in 0.5 mm increments.
- Enable wiping or a small coast at the end of each move if your slicer offers it.
More retraction is not always better. Past a certain distance the filament softens inside the heat break and the extruder starts to grind, which looks like random under-extrusion mid-print.
Step 4: travel and speed
Strings appear when the nozzle crosses open space while still dripping. Reduce the number of long travel moves by turning on a combing mode that keeps the nozzle over printed areas, and raise travel speed to at least 150 mm/s so there is less time to ooze. Print order matters too: a part with two separate towers will always string more than one printed as a single body.
Cleaning up what remains
A little residual stringing is normal for PETG. A quick pass with a hot air gun on its lowest setting, held a hand's width away, shrinks fine strings without marking the surface. For a stubborn blob, a deburring tool or a sharp craft knife works better than sandpaper, which tends to smear the plastic.
What I settled on
For a 0.4 mm nozzle on a direct drive machine, I print dried PETG at 235 °C, retract 1.2 mm at 35 mm/s, travel at 180 mm/s and keep the first layer bed at 80 °C, dropping to 70 °C afterwards. These numbers are a starting point, not a recipe. Brands differ, and even different colours from the same brand can behave differently because of the pigments.
Keep notes on a card taped to the printer. When a new spool arrives, print the same tower and write the best temperature and retraction directly on the spool edge. It takes ten minutes and saves hours later. If you are printing parts that move against each other, read the notes on hinge clearances as well, since stringing inside a gap can fuse a joint.